应用化学 ›› 2025, Vol. 42 ›› Issue (11): 1479-1490.DOI: 10.19894/j.issn.1000-0518.240374

• 研究论文 • 上一篇    下一篇

聚(3,4-亚乙二氧基噻吩)-聚(苯乙烯磺酸)/聚乙烯醇半互穿网络聚合物的制备及其性能

吉汪尧, 菅晓霞(), 韩佩瑶, 张翔   

  1. 南京理工大学化学与化工学院,南京 210094
  • 收稿日期:2024-11-18 接受日期:2025-09-25 出版日期:2025-11-01 发布日期:2025-12-05
  • 通讯作者: 菅晓霞

Preparation and Properties of Poly(3,4-ethylenedioxythiophene)- Poly(styrenesulfonate)/Polyvinyl Alcohol Semi-Interpenetrating Polymer Network

Wang-Yao JI, Xiao-Xia JIAN(), Pei-Yao HAN, Xiang ZHANG   

  1. School of Chemistry and Chemical Engineering,Nanjing University of Science and Technology,Nanjing 210094,China
  • Received:2024-11-18 Accepted:2025-09-25 Published:2025-11-01 Online:2025-12-05
  • Contact: Xiao-Xia JIAN
  • About author:jxx259@163.com

摘要:

采用线性聚3,4-乙烯二氧噻吩/聚苯乙烯磺酸(PEDOT∶PSS)与交联聚乙烯醇(PVA),以不同质量比制备了系列半互穿网络结构的导电聚合物PEDOT∶PSS/PVA。 采用傅里叶变换红外光谱(FT-IR)、拉曼光谱、X射线衍射(XRD)、热失重分析(TGA)、四探针测试和电子式万能试验机对导电聚合物进行性能表征。 结果表明,PVA与PEDOT∶PSS能够在一定范围内良好相容,通过氢键作用形成均一形貌,随着PVA质量分数的增大,PEDOT∶PSS/PVA会发生相反转,当PVA质量分数为40%时,PEDOT∶PSS/PVA电导率为1.85 S/m,其拉伸强度达到6.83 MPa,断裂伸长率为22.89%,PEDOT∶PSS/PVA可以代替导线点亮小灯泡,且电阻随温度变化的幅度较大,对温度变化敏感。

关键词: 聚3, 4-乙烯二氧噻吩/聚苯乙烯磺酸, 聚乙烯醇, 导电凝胶

Abstract:

A series of conductive polymers poly(3,4-ethylenedioxythiophene)-poly(styrenesulfonate)/polyvinyl alcohol (PEDOT∶PSS/PVA) with semi-interpenetrating network structure were prepared by using linear poly(3,4-ethylenedioxythiophene)/polystyrene sulfonic acid (PEDOT∶PSS) and cross-linked polyvinyl alcohol (PVA) with different mass ratios. The properties of the conductive polymers were characterized by Fourier transform infrared spectrometer (FT-IR), Raman spectrometer, X-ray diffractometer (XRD), thermogravimetric analyzer, four-probe tester and electronic universal testing machine. The results show that PVA and PEDOT∶PSS can be well compatible in a certain range, and form a uniform morphology through hydrogen bonding. With the increase of PVA mass fraction, PEDOT∶PSS/PVA will reverse. When the mass fraction of PVA is 40%, the conductivity of PEDOT∶PSS/PVA is 1.85 S/m, the tensile strength is 16.83 MPa, and the elongation at break is 22.89%. PEDOT∶PSS/PVA can replace the wire to light a small bulb, and the resistance varies greatly with temperature, which is sensitive to temperature change.

Key words: Poly(3, 4-ethylenedioxythiophene)/polystyrene sulfonic acid, Polyvinyl alcohol, Electrographic gel

中图分类号: