应用化学 ›› 2016, Vol. 33 ›› Issue (4): 430-435.DOI: 10.11944/j.issn.1000-0518.2016.04.150278

• 研究论文 • 上一篇    下一篇

秸秆预处理工艺对秸秆基人造板性能的影响

靳璇ab,李赢ab,李新a,余志科a,张天宇a,丁重阳b,石刚a*()   

  1. a江南大学化学与材料工程学院 江苏 无锡 214122
    b江南大学粮食发酵工艺与技术国家工程实验室 江苏 无锡 214122
  • 收稿日期:2015-08-06 接受日期:2015-12-09 出版日期:2016-04-01 发布日期:2016-04-01
  • 通讯作者: 石刚
  • 基金资助:
    国家自然科学基金(21401079)江苏省自然科学基金(BK20140158)高等学校博士学科点专项科研基金(20130093120003)资助项目

Effect of Pretreatment Methods of Rice Straw on Straw Board Properties

JIN Xuanab,LI Yingab,LI Xina,YU Zhikea,ZHANG Tianyua,DING Zhongyangb,SHI Ganga*()   

  1. aSchool of Chemical and Material Engineering,Jiangnan University,Wuxi,Jiangsu 214122,China
    bNational Engineering Laboratory for Cereal Fermentation Technology,Jiangnan University,Wuxi,Jiangsu 214122,China
  • Received:2015-08-06 Accepted:2015-12-09 Published:2016-04-01 Online:2016-04-01
  • Contact: SHI Gang
  • Supported by:
    Supported by the National Natural Science Foundation of China(No.21401079), Jiangsu Province Science Foundation for Youths(No.BK20140158), Research Fund for the Doctoral Program of Higher Education(No.20130093120003)

摘要:

随着木材工业的快速发展,以及木材原料的日益减少,利用农作物秸秆代替木材生产复合材料十分必要。 本文以水稻秸秆为原料,以脲醛树脂为粘合剂,通过湿热法、偶联剂表面化学改性的方法,对秸秆表面进行改性,从而提高了树脂和秸秆之间的结合力,探索了水稻秸秆板的制作工艺。 实验表明较好的制备工艺为:温度150 ℃,压强15 MPa,热压时间8 min,树脂胶粉和水的质量比为1:1,脲醛树脂胶含量为15%(质量分数),发现秸秆表面预处理采用γ-缩水甘油醚氧丙基三甲氧基硅烷(KH560)偶联剂后,所制得的秸秆板的诸多性能优于未经预处理及采用γ-氨丙基三乙氧基硅烷(KH550)进行改性后所制的秸秆板。

关键词: 秸秆, 表面改性, 脲醛树脂, 偶联剂

Abstract:

The renewable lignocellulosic sources for biocomposites have received much attention in recent years because of the shortage of forest resources. The surface of rice straw was pretreated through humid-heat and chemical modification by coupling reagent which could improve the adhesion capacity between urea formaldehyde resin and rice straw. Meanwhile, the process of fabricating straw board was explored in this paper. The experimental data shows that the straw boards with perfect properties are prepared under the temperature of 150 ℃, the pressure of 15 MPa, the hot pressing time of 8 min, the mass ratio of resin powder to water of 1:1, and the urea formaldehyde resin adhesive content of 15%(mass fraction). The straw boards prepared by 3-glycidyloxypropyltrimethoxysilane(KH560) as surface modification reagent show better properties than those by KH550 and untreated rice straw.

Key words: straw, surface modification, urea formaldehyde resin, coupling agent